PRODUCT DATA of AA2618-T851 |
Material | AA2618-T851 |
General Information | The 2618 aluminium alloy is a wrought alloy which responds to an age-hardening heat treatment. |
Chemical Composition | Si 0.1-0.25, Fe 0.9-1.3, Cu 1.9-2.7, Mg 1.3-1.8, Zn 0.1, Ni 0.9-1.2, Ti 0.04-0.1, Others: Each 0.05 Total 0.15, Rem. Al |
Name of Manufacturer | Pechiney Rhenalu Issoire |
EXPERIENCE IN PRACTICE |
---|
Development Status | Commercial Product |
Cost Range | Low |
Equivalent Designations | AA 2618; AlCu2Mg1.5Fe1Ni1; A-U2GN, AU2GN; AlCu2Mg2Ni; LW3.1924; H16, Hiduminium RR; DTD717A, 724, 731A, 731B; 745A, 5084A, 5014A |
PHYSICAL PROPERTIES |
---|
Crystal Structure | Face centered cubic (fcc) |
Specific Gravity | 2.76 |
Magnetic Properties | Nonmagnetic |
MECHANICAL PROPERTIES |
---|
Ultimate Tensile Strength | 441 MPa Data Quality: Typical Data |
Proof Stress (0.2%) | 372 MPa Data Quality: Typical Data |
Elongation | 10% Data Quality: Typical Data |
THERMAL PROPERTIES |
---|
Thermal Conductivity | 147 W/m.K |
Thermal Expansion Coefficient | 22.3 µstrain/°C Remark: @ temperature 20-100 C |
Melting Range | 549 to 638 °C Solidus - Liquidus |
RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
---|
General Corrosion Status | Requires specific corrosion protection |
Stress Corrosion Status | High Resistance to SCC: Table 1 Remark: Resistant (ECSS-Q-ST-70-36C) Tempers T6 and T8 are considered to be Table 1 alloys Data Quality: Design Data |
Bimetallic Corrosion | Can be used in a non-controlled environment with: Al+alloys, Cd, Sn-Pb alloys, Sn, Pb
Can be used in a clean room environment with: as above and Mg, Ni, Monel, Inconel, Ni-Mo alloys, 300 series SS, 400 series SS, Ti and Ti alloys, Zn, Be Needs specific measures: All others Remark: ECSS-Q-ST-70C Rev.1 table 5.1 Data Quality: Design Data |