All data is for information only------(Home)
PRODUCT DATA of AA3105-H12
MaterialAA3105-H12
Processing and AssemblyH12 temper: product is strain-hardened (quarter hard) to obtain the desired strength without supplementary thermal treatment
Chemical Composition0.2-0.8Mg, 0.3-0.8Mn, rem Al
EXPERIENCE IN PRACTICE
Development StatusCommercial Product
Lot ReproducibilityGood
Equivalent DesignationsA-M1G, Al Mn1Mg1, D4S
Space ExperienceGood
PHYSICAL PROPERTIES
Crystal StructureFace centered cubic (fcc)
Specific Gravity2.72
Magnetic PropertiesNonmagnetic
ELASTIC PROPERTIES
Tensile Modulus69.5 GPa
Shear Modulus28.1 GPa
MECHANICAL PROPERTIES
Ultimate Tensile Strength117 to 159 MPa
Proof Stress (0.2%)90 MPa(minimum)
Data Quality: Minimum specification data
Elongation3 to 10 %
Shear Strength115 MPa
ELECTRICAL PROPERTIES
Electrical Volume Resistivity4.1e-8 ohm.m
Electrical Conductivity42 %IACS
THERMAL PROPERTIES
Thermal Conductivity160 W/m.K
Thermal Expansion Coefficient23.9 µstrain/°C
Specific Heat0.893 J/g.K
Melting Range629 to 654 °C
RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY
General Corrosion StatusNo specific corrosion protection required
Stress Corrosion StatusHigh Resistance to SCC: Table 1
Data Quality: Design Data
EMF vs SCE-0.76 V
Bimetallic CorrosionCan be used in a non-controlled environment: Al alloys, Cd
Can be used in a clean room environment: Mg, Sn-Pb alloys (all), Sn, Pb, Zn, Be
Needs specific measures: All others
Data Quality: Design Data