PRODUCT DATA of CDA 706 |
Material | CDA 706 |
General Information | Typical data from standards handbook of copper and copper alloys (Copper.org) @ Room Temperature |
Chemical Composition | Cu-10Ni-1.4Fe |
EXPERIENCE IN PRACTICE |
---|
Equivalent Designations | C70600; CuNi10Fe1Mn; CW352H; 2.0872; CN102; CDA706 ; copper-nickel 10% |
PHYSICAL PROPERTIES |
---|
Specific Gravity | 8.94 |
ELASTIC PROPERTIES |
---|
Tensile Modulus | 124 GPa |
Shear Modulus | 46.9 GPa |
ELECTRICAL PROPERTIES |
---|
Electrical Volume Resistivity | 1.91e-7 ohm.m |
THERMAL PROPERTIES |
---|
Thermal Conductivity | 45 W/m.K |
Thermal Expansion Coefficient | 17.1 µstrain/°C |
Specific Heat | 0.377 J/g.K |
Melting Range | 1100 to 1150 °C |
RELEVANT PROPERTIES FOR USE IN SPACE COMMUNITY |
---|
Stress Corrosion Status | High Resistance to SCC: Table 1
Remark: in the 50% cold rolled condition only Remark: acc. to ECSS-Q-ST-70-36C Data Quality: Design Data |